SOL RESEARCHHUBZONE SMALL BUSINESSCAGE 44KM9Also on iOS & Android
RESEARCH PAPERP2UNCLASSIFIED

Thermal Expansion Mismatch and Power Module Reliability

CTE mismatch, failure mechanisms, lifetime models and qualification evidence for silicon carbide power modules and their cold plates

SOL Engineering Services
PUBLISHED
READING TIME
34 min
Download PDF

Executive Summary

Thermal expansion mismatch is a principal wear-out driver in thermally cycled silicon carbide (SiC) power modules, and the strongest published evidence for reducing it comes from low-CTE baseplates. In finite-element modeling by the National Renewable Energy Laboratory (NREL), the strain energy density per cycle in a 5 mm baseplate stack is 0.18 MPa for aluminum silicon carbide (AlSiC), 1.94 MPa for copper and 3.93 MPa for aluminum.1 A tested liquid-cooled AlSiC heat sink, which the authors compare with a conventional stack, completed 1,800 cycles from −40 to 150 °C without failure, and the authors report a lifetime improvement of at least 18 times.2

Five findings support the paper’s conclusions.

  • Material values. Copper expands at 16.5 to 17 ppm/K, aluminum at 22.2 to 25 ppm/K, SiC dies at 3.4 to 4 ppm/K, aluminum nitride at 4.5 to 4.7 ppm/K and silicon nitride at 2.5 to 3.2 ppm/K. Alumina expands at 6.8 to 8.2 ppm/K, so the range of 3 to 4.5 ppm/K applies to SiC, aluminum nitride and silicon nitride and excludes alumina (Table 2). Copper and aluminum expand four to eight times as much as SiC and silicon nitride.

  • Failure modes. Bond-wire lift-off and solder fatigue are the most frequently reported packaging failures, and the one that appears first depends on the temperature gradient and the cycle duration.34 SiC raises the stress in die-attach solder: a published comparison finds a corner stress of 70 MPa for SiC against 32.1 MPa for silicon at a 120 °C temperature swing, and attributes the difference mainly to SiC’s elastic modulus of 501 GPa against 162 GPa, with CTE a minor factor.5

  • Lifetime models. The LESIT, CIPS 2008 and Semikron Danfoss models express cycles to failure through junction temperature swing, mean or maximum junction temperature and pulse duration. None contains a CTE term, so mismatch enters only through the fitted constants. Coffin-Manson and the finite-element physics-of-failure models act on strain and take CTE as an input (Table 5). In one field case, two IGBT failures followed about 3.2×10⁸ accumulated cycles against about 5×10⁸ expected from a LESIT extrapolation, and the author questions the extrapolation.6

  • Low-CTE evidence. The public record contains modeling that favors AlSiC by a factor of 11 to 22 in strain energy density (derived), one tested AlSiC liquid-cooled heat sink with an improvement of at least 18 times, and test evidence at the substrate level (Table 6). The sources reviewed contain no published life test that varies cold plate CTE in a SiC module while holding other variables constant.

  • Qualification. The guideline AQG 324 of the European Center for Power Electronics (ECPE) defines short and long power cycling and a thermal shock test, with failure criteria of +5 percent drain-source voltage and +20 percent thermal resistance as reported by a vendor white paper.7 IEC 60749-34-1:2025, JEDEC JESD22-A104F.01 and MIL-STD-810H Method 503.7 address power cycling, temperature cycling and air temperature shock, and none sets a fixed cycle count for a ground vehicle mission (Table 7).

The paper recommends that the CF-JET effort measure and report the in-plane CTE of the finished target plate, including the plated coolant face, from 25 to 175 °C; set a mismatch target against the selected ceramic; and validate the module with power cycling and thermal shock using the AQG 324 failure criteria.

1. Introduction and Scope

A SiC power module is a stack of dissimilar materials bonded at high temperature and operated across a temperature range that exceeds 100 K in service. Each material expands at a different rate, and each change in temperature loads the bonded interfaces. This paper describes how thermal expansion mismatch limits the life of SiC power modules and what evidence supports using low-CTE materials in the module and its cold plate. The intended readers are program managers at the U.S. Army DEVCOM Army Research Laboratory, engineers at the Ground Vehicle Systems Center (GVSC), university co-investigators and industry partners who specify, design and test cooling hardware for ground vehicle power electronics.

The scope covers the coefficients of thermal expansion (CTE) of SiC dies, ceramic substrates, solder and sintered joints, baseplates and cold plates; the failure mechanisms that thermal cycling produces; the lifetime models that predict cycles to failure; and the qualification standards that apply. Four questions organize the paper. Which failure modes dominate SiC module life? How do lifetime models quantify CTE mismatch? What evidence shows that low-CTE heat sinks or cold plates extend module life? Which qualification standards apply? Table 1 states four claims that this paper tests and the verdict on each.

Table 1. Four claims tested and the verdicts

Claim Verdict Basis for the verdict
Copper expands at about 17 ppm/K. Supported Three sources reviewed give 16.5 ppm/K for copper, and one patent gives about 17 ppm/K.891011
Aluminum expands at about 23 ppm/K. Supported within a range Research sources give 22.2 and 22.7 ppm/K, and a patent gives about 25 ppm/K. The value depends on alloy and test range.12
SiC and ceramic substrates expand at about 3 to 4.5 ppm/K. Supported for SiC, silicon nitride and aluminum nitride; alumina is higher SiC dies are 3.4 to 4 ppm/K, silicon nitride 2.5 to 3.2 ppm/K and aluminum nitride 4.5 to 4.7 ppm/K. Alumina is 6.8 to 8.2 ppm/K.13
CTE mismatch is a leading cause of power module failure. Supported as a leading wear-out driver in cycled service; the share of field failures is not quantified Test and review sources tie the two most frequent packaging failures to CTE differences. Survey statistics rank power semiconductors as the most fragile components and do not isolate CTE.1415

Verdicts apply to the sources reviewed. Table 4 gives the evidence on the fourth claim.

The CF-JET effort, proposed by SOL Engineering Services, LLC, applies an additively manufactured, liquid-cooled jet-impingement cold plate with an optimized carbon fiber target plate to the thermal management of SiC power modules.16 The proposal places perpendicular pitch-based carbon fiber inserts under each die and seals the coolant face with a thin electroplated metal layer. These are design proposals. The paper tests the reliability implications of those proposals against independently published results and states the open questions. Figure 1 shows the module layers and their expansion coefficients.

Figure 1. Layers of a SiC power module, their coefficients of thermal expansion and the cycling load

Layers of a SiC power module, their coefficients of thermal expansion and the cycling load

The coefficient ranges are those in Table 2. The diagram is schematic and not to scale.

2. Material Properties and the Mismatch They Create

2.1 Copper and aluminum expand four to eight times as much as SiC and silicon nitride

Table 2 lists the CTE, thermal conductivity and elastic modulus of the module materials as reported in the sources reviewed. Figure 2 plots the CTE ranges. The ranges arise from differences in alloy, measurement temperature range and source. Rogers reports its ceramic values over 20 to 300 °C, and NREL’s finite-element inputs vary with temperature.1718

Table 2. Coefficient of thermal expansion, thermal conductivity and elastic modulus of module materials

Material CTE (ppm/K) Thermal conductivity (W/m·K) Elastic modulus (GPa) Notes
Silicon die19 2.6 to 3.2 130 to 148 162 NREL, patent and Hu et al. values.20
SiC die21 3.4 to 4.0 370 501 Hu et al. list 3.4 in a table and a patent lists about 4.22
Silicon nitride 2.5 to 3.2 Not listed 300 Rogers, NREL.
Aluminum nitride 4.5 to 4.7 155 330 Same value in four sources.
Alumina 6.8 to 8.2 25 360 Range spans three sources.
AlSiC baseplate 8.0 to 8.4 180 Not listed Pahinkar et al., Vincotech.
Copper 16.5 to 17.0 401 Not listed Baseplate and metallization.
Aluminum 22.2 to 25.0 Not listed Not listed Alloy dependent.
SnAg or SAC305 solder 21.6 to 22.1 62 (SnAg) Not listed Vincotech, NREL.

Sources: Vincotech (vendor technical paper), NREL presentation slides, Pahinkar et al., Hu et al., Rogers (vendor data sheet) and two U.S. patents. Cells marked Not listed indicate that the sources reviewed give no value.

Figure 2. CTE ranges of module materials across the sources reviewed

CTE ranges of module materials across the sources reviewed

Black bars show the range of reported values; the red bar and dashed line mark the SiC die. Values are reported, with ranges compiled in this paper.

Copper at 16.5 ppm/K expands 4.1 times as much as a SiC die at 4 ppm/K and 5.9 times as much as silicon nitride at 2.8 ppm/K. Aluminum at 22.2 ppm/K expands 5.6 and 7.9 times as much.23 Solder alloys at 21.6 to 22.1 ppm/K expand at about the rate of aluminum. The first three claims in Table 1 follow from these values. The one qualification is alumina, which expands at about twice the rate of SiC and lies between SiC and copper.

2.2 Joining layers experience the largest free mismatch

Table 3 converts the CTE values into the free thermal strain mismatch that each joint must accommodate over a 100 K temperature swing. The figure shows the driving mismatch and not the strain in the joint, because compliance, geometry, creep and the thickness of each layer determine how much of the mismatch the joint absorbs. The solder layer between a die and its substrate experiences the largest mismatch in the stack, 17.6 to 19.3 ppm/K, because solder expands at 21.6 to 22.1 ppm/K against 2.8 to 4 ppm/K for the die.

Table 3. Free CTE mismatch at the joints of a SiC power module (derived)

Joint Materials and CTE (ppm/K) Mismatch Δα (ppm/K) Free strain mismatch at ΔT = 100 K (%)
Solder layer to SiC die SAC305 21.6; SiC 4.0 17.6 0.176
Solder layer to silicon die SnAg 22.1; silicon 2.8 19.3 0.193
Die to copper metallization SiC 4.0; copper 16.5 12.5 0.125
Copper cladding to silicon nitride Copper 16.5; silicon nitride 2.8 13.7 0.137
Copper cladding to aluminum nitride Copper 16.5; aluminum nitride 4.5 12.0 0.120
Copper cladding to alumina Copper 16.5; alumina 8.2 8.3 0.083
Silicon nitride to copper baseplate 2.8; 16.5 13.7 0.137
Silicon nitride to aluminum baseplate 2.8; 22.2 19.4 0.194
Silicon nitride to AlSiC baseplate 2.8; 8.0 5.2 0.052
Aluminum nitride to copper baseplate 4.5; 16.5 12.0 0.120
Aluminum nitride to AlSiC baseplate 4.5; 8.0 3.5 0.035
Alumina to copper baseplate 8.2; 16.5 8.3 0.083
Alumina to aluminum baseplate 8.2; 22.2 14.0 0.140
Alumina to AlSiC baseplate 8.2; 8.4 0.2 0.002

Derived from the values in Table 2 as Δα = |α1 − α2| and strain mismatch = Δα × 100 K. Ceramic-only values overstate the mismatch against copper and aluminum baseplates, because the copper cladding raises the net CTE of the substrate.

The baseplate joint matters because of its size. Vincotech states that the stress is higher in the joint between the copper baseplate and the substrate than in the die joint, because of the larger difference between the net CTEs of an alumina substrate and a copper baseplate, and because the baseplate joint is much larger and therefore more prone to failure in thermal cycling.24 The same paper reports that delamination starts at the edges of the solder joint and expands inward, and that a copper baseplate bows the module concavely as temperature rises, which opens a gap to the heat sink and can push thermal grease out.25 These are vendor statements, and they match the direction of the modeling results in Table 6. Figure 3 compares each ceramic with each baseplate.

Figure 3. Free CTE mismatch between ceramic substrates and baseplates, in ppm/K (derived)

Free CTE mismatch between ceramic substrates and baseplates, in ppm/K (derived)

Values are absolute differences between the coefficients in Table 2, as in Table 3. The value marked with an asterisk is calculated here from 22.2 and 4.5 ppm/K and does not appear in Table 3.

AlSiC reduces the baseplate mismatch to 0.2 to 5.2 ppm/K depending on the ceramic. Silicon nitride is the best match to a SiC die and has a larger mismatch with an AlSiC baseplate (5.2 ppm/K) than alumina does (0.2 ppm/K). The material that matches the die best therefore does not always match the baseplate best, and the choice of substrate ceramic and baseplate requires evaluation as a pair.

2.3 Stiffness and conductivity change the effect of CTE in SiC

SiC and silicon have similar CTE values and differ in two other properties. The elastic modulus of SiC is 501 GPa against 162 GPa for silicon, and its thermal conductivity is 370 against 130 W/m·K.26 Hu et al. use a finite-element model validated against power cycling tests on silicon IGBT modules to compare the solder layer under a SiC die and a silicon die with the same junction temperature profile. At a 120 °C swing and a mean junction temperature of 90 °C, the corner stress is 70 MPa for SiC and 32.1 MPa for silicon, a ratio of 2.2, and the accumulated creep energy density is 15,891 J/m³ against 4,459 J/m³, a ratio of 3.6.27 The authors identify the elastic modulus as the dominant factor and state that the CTE mismatch of SiC with solder is slightly smaller than that of silicon.28

This result refines the claim that CTE mismatch causes failure. CTE sets the free strain mismatch, and the stiffness of the bonded materials converts that strain into stress. A stiffer die constrains the solder more tightly, and the same strain produces more stress and creep. The implication for a cold plate is that reducing CTE mismatch lowers the strain input, and the remaining stress depends on the stiffness of the die, substrate and baseplate.

3. Failure Modes in SiC Power Modules

3.1 Bond-wire lift-off and solder fatigue lead the reported packaging failures

The sources reviewed agree on the list of packaging failure modes and differ on their order. NREL researchers state that wire-bond lift-off and solder delamination are the most frequent packaging failures and that thermal and power cycling stress them most often.29 In their thermal cycling of a SiC MOSFET from −40 to 175 °C, a 215 °C difference, the maximum change in on-resistance after 1,500 cycles was 15 percent. The authors speculate that solder crack growth or wire-bond lift-off caused the increase, and the test used a single device per condition.30

The Semikron Danfoss application note lists chip solder fatigue, bond-wire heel cracks or lift-off, and a combination of bond-wire failure with degradation of the top-side metallization. The note states that the mode that triggers first depends on the temperature gradient and the cycle duration, and that baseplate solder fatigue is a separate mechanism that the power cycling models do not cover.31 A Wolfspeed white paper adds failure modes for sintered die attach (void formation and silver migration) and for copper clips (fatigue at bond interfaces and at geometric transitions), and states that a rise in drain-source voltage accompanies wire-bond lift-off in silicon modules.32 Table 4 summarizes the modes, their location and the test that targets each.

Table 4. Thermal cycling failure modes in power modules, their drivers and the tests that target them

Location and mode Driver Test that targets it Evidence and source type
Bond wire: lift-off and heel cracking CTE difference between the aluminum wire (aluminum is 22.2 to 25 ppm/K) and the die; temperature swing; current per wire Short power cycling (PCsec, ton under 5 s) Most frequent packaging failure in NREL testing; modeled in LESIT and CIPS 2008.3334
Top-side metallization degradation Cyclic strain at the die surface, combined with bond-wire failure Power cycling Semikron Danfoss application note (vendor).35
Die-attach solder: fatigue and delamination Solder expands 17.6 to 19.3 ppm/K more than the die; stiff SiC die raises stress Short power cycling Modeled and tested on silicon; SiC comparison by modeling.36
Sintered die attach: voids, silver migration Cyclic strain and temperature Power cycling Wolfspeed white paper (vendor).37
Copper clip: fatigue at bond interfaces CTE difference at the clip joint; geometry Power cycling Wolfspeed white paper (vendor).38
Substrate-to-baseplate solder: fatigue, delamination from the edge Net substrate CTE against baseplate CTE; large joint area Long power cycling (PCmin, ton over 15 s) Vincotech technical paper (vendor); AQG 324 target as reported by a vendor page.3940
Ceramic substrate: fracture, copper-to-ceramic delamination Copper 16.5 ppm/K against ceramic 2.8 to 8.2 ppm/K; ceramic fracture toughness Thermal shock (TST in AQG 324) Peer-reviewed test, harsher than automotive conditions.41
Baseplate bowing and grease pump-out Bimetallic effect of a copper baseplate Not stated in the source Vincotech technical paper (vendor).42

3.2 SiC raises the stress in die-attach solder

Hu et al. cite earlier work that considers the in-service solder lifetime under a SiC die to be one third of the silicon benchmark, and they report their own, smaller estimate. At a temperature swing of 90 °C the lifetime of the SiC device is 60 percent of the silicon device, and the ratio approaches 1 as the swing increases.43 Creep energy at a 90 °C swing is about 2.4 times higher for SiC and falls to about 1.2 times at large swings.44 The experimental results of the paper cover silicon IGBT modules only, with 6,200 to 53,000 cycles to failure across the tested conditions and a failure criterion of a 20 percent rise in thermal resistance, so the SiC lifetime estimates come from the validated model and no SiC life test supports them.45

Wolfspeed reaches a similar conclusion in qualitative terms. Its white paper states that the higher stiffness and thermal conductivity of SiC amplify mismatch stress at interfaces, and that long power cycling pulses spread heat through the full stack so that more material experiences the mismatch.46 The vendor reports that its YM module family uses sintered die attach and active metal brazed (AMB) substrates for better CTE matching, and that the family achieves three times the power cycles of the best competitor in the same footprint, with no absolute cycle count in the text.47

3.3 Substrate cracking depends on the ceramic and the thermal shock range

Choe et al. tested copper-clad AMB substrates of alumina, aluminum nitride and silicon nitride between −50 and 250 °C with 30 minute dwells at each temperature. The alumina and aluminum nitride substrates fractured within the ceramic by the first inspection at 10 cycles, and the silicon nitride substrates survived 1,000 cycles with either nickel or nickel-phosphorus plating.48 The authors attribute the difference to the higher fracture toughness of silicon nitride, listed as 7 MPa·m^½.49 Two samples were tested per material combination, and the upper temperature of 250 °C exceeds the maximum junction temperatures of 125 to 175 °C in typical SiC power cycling profiles.50 The test shows the ranking of the ceramics and gives no life figure for a vehicle.

The same paper bears on any plated surface on a low-CTE material. On the surviving silicon nitride substrates the nickel layer, about 7 µm thick, showed no cracking after 1,000 cycles, and the nickel-phosphorus layer developed a thin crack.51 The result indicates that the plating chemistry affects survival under thermal shock.

3.4 CTE mismatch is a leading wear-out driver, and field statistics do not isolate its share

The fourth claim in Table 1 divides into a mechanism claim and a statistical claim. The mechanism claim is supported. NREL researchers link wire-bond lift-off and solder delamination to CTE differences between the device and package layers, Semikron Danfoss states that temperature swings acting on the differing CTEs of the package materials cause wear-out of the interconnections, and Wolfspeed states that the layered materials respond differently to thermal cycling.525354

The statistical claim has weaker support. An industry survey of power electronic converters ranked power semiconductor devices as the most fragile components and named environment, transients and heavy loads as the main stresses; the survey is subjective, and its authors drew on respondents from several sectors.55 A reliability review by Wang and Blaabjerg covers failure mechanisms, physics-of-degradation and mission profiles for power electronics and does not rank CTE mismatch against other causes in the portions reviewed.56 A figure quoted in secondary literature attributes 55 percent of electronic failures to temperature, steady-state and cyclical combined.57 The underlying survey was not located, and the figure covers electronics in general. The sources reviewed therefore support CTE mismatch as a leading wear-out driver in modules that cycle in temperature and contain no field failure share attributed to it.

4. Lifetime Models and How They Treat Mismatch

4.1 Empirical models express life through temperature swing, and mismatch enters implicitly

Table 5 compares the lifetime models used for power modules. The solder-joint models, Coffin-Manson and its Norris-Landzberg modification, relate cycles to failure to the plastic strain range or temperature range, and Escobar and Meeker describe Coffin-Manson as the most commonly used model for accelerating thermal cycling failures.58 Norris and Landzberg added terms for cycling frequency and maximum temperature. Reported fitted exponents are 1.9 for the temperature range and one third for frequency in eutectic tin-lead solder, and Pan et al., as quoted in a vendor forum thread, report 2.65, 0.136 and an activation temperature of 2,185 K for tin-silver-copper solder.5960 Vasudevan and Fan propose a three-parameter modified Coffin-Manson model for lead-free solder that they fit to 17 pairs of temperature cycle tests.61

The power-cycling models take junction temperature swing as the load variable. The LESIT project tested standard modules from several manufacturers and identified bond-wire lifting as the predominant failure mechanism,62 and the CIPS 2008 model by Bayerer and colleagues applies multiple regression to a large body of power cycling data from several generations of IGBT modules.6364 The CIPS 2008 variables are temperature swing, junction temperature, power-on time, chip thickness, bonding technology, bond-wire diameter, current per wire bond and package type. For a fixed module technology and voltage class, the authors reduce the key factors to temperature swing, junction temperature, power-on time and current per wire bond.65 Neither model contains a CTE term. The CTE of each layer is part of the module construction that the fitted constants represent, so the effect of a change in baseplate or substrate material is not predicted by these models and requires new test data.

Table 5. Lifetime models for thermally cycled power modules and their treatment of CTE mismatch

Model Form and variables Basis Stated validity or limits Treatment of CTE
Coffin-Manson Cycles to failure as a power law of plastic strain range or temperature range Low-cycle fatigue of metals and solder joints Exponent depends on alloy and joint design Through plastic strain range, which mismatch produces
Norris-Landzberg Coffin-Manson acceleration factor with frequency and maximum temperature terms Chamber thermal cycling of solder joints Parameters differ for tin-lead and lead-free solder Same as Coffin-Manson
LESIT Cycles to failure against temperature swing at three mean junction temperatures Power cycling of commercial IGBT modules, mid-1990s Extrapolation to 5×10⁸ cycles was questioned in one field case None explicit
CIPS 2008 Regression on temperature swing, junction temperature, pulse time, chip thickness, bonding, wire diameter, current per wire, package Power cycling data from several IGBT generations Fixed technology and voltage class; evaluated for 1200 V IGBT4 modules None explicit
Semikron Danfoss AN 21-001 LESIT-based Arrhenius and Coffin-Manson model with pulse time, chip thickness and low-temperature terms Power cycling, Weibull statistics, 15 percent failure probability Swing 50 to 120 K (DC test); 30 to 63 K (inverter test); mean junction temperature up to 400 K None explicit; separate parameter sets for baseplate, baseless and sintered modules
Finite-element physics of failure Stress, creep strain and strain energy density per cycle, converted to life with a fatigue law Material properties, geometry, load profile Requires calibration to tests Explicit, as an input
Mission-profile damage summation Rainflow counting of junction temperature profiles and cumulative damage Electro-thermal simulation of the mission No equations or parameters published in the vendor white paper Through the underlying lifetime model

Sources: Escobar and Meeker; Vasudevan and Fan; Held et al.; Bayerer et al.; Wintrich (Semikron Danfoss); Hu et al.; Wolfspeed white paper. The closed-form equation of CIPS 2008 and its coefficients are in the source paper, which this study did not obtain in full text.

4.2 The Semikron Danfoss model shows the fitted structure and the validity limits

The Semikron Danfoss application note, revised in July 2024, describes the most explicit public parameter set for a LESIT-based model. It uses a temperature-swing exponent of −4.3, an activation energy of 4.5×10⁻²⁰ J (0.28 eV) for modules with and without baseplates, and 2.54×10⁻²⁰ J (0.16 eV) for sintered chips, with time exponents of −0.75, −0.7 and −1.21 for the three constructions.6667 The note states that its figures represent a 15 percent failure probability, uses Weibull statistics, and defines end of life as a 20 percent rise in forward voltage, thermal resistance or temperature swing.68

The Wolfspeed white paper cites a different electrical criterion, a 5 percent rise in drain-source voltage, and the same 20 percent rise in thermal resistance, both attributed to AQG 324.69 The two criteria differ, and a lifetime stated without its criterion cannot be compared across sources. The validity ranges are a second limit. The note states ranges of 50 to 120 K for temperature swing in DC tests, 0.07 to 60 s for pulse time, 70 to 310 µm for chip thickness and 600 to 1,700 V for voltage class, with a mean junction temperature of up to 400 K (127 °C).70 A module cooled with 105 °C coolant has 22 K between the coolant and the upper validity limit of the mean junction temperature, which leaves a small margin for the junction-to-coolant temperature rise.7172 The note is titled for IGBT product lines, and the construction list it gives includes MOSFET.73

4.3 Extrapolation of empirical curves beyond test conditions is a documented concern

Künzi extrapolated the LESIT results to an expected life of about 5×10⁸ cycles of 320 ms duration. A booster power supply accumulated about 3.2×10⁸ such cycles, which the author calls considerably below the expected lifetime, and he questions whether such an extreme extrapolation is appropriate.74 The same notes report two IGBT failures within a month after 3.5 years of energy-saving operation and judge the 100 s cycle, with a 56 K peak-to-peak swing, the most likely cause.75 The case involves silicon IGBTs in a stationary application. It illustrates the risk of applying a model fitted at high swings and short test times to low swings and long service times, and it gives no information on SiC modules.

The Wolfspeed white paper states that power cycling testing has no fixed pass or fail cycle count and that the model is empirical, relating junction temperature swing, maximum junction temperature and pulse time to cycles to failure through parameter sweeps. Typical test profiles in the paper use swings of 75 to 125 °C and maximum junction temperatures of 125 to 175 °C.76 A mission profile is converted to junction temperature cycles by electro-thermal simulation, counted by rainflow analysis and combined by cumulative damage.77

4.4 Physics-of-failure models take CTE as an input

Finite-element models compute the stress and strain that mismatch produces. Hu et al. use a two-dimensional model with 120 µm solder and report creep strain per cycle and accumulated creep energy density, and NREL reports strain energy density per cycle for baseplate and ceramic combinations.7879 These models take CTE, elastic modulus and geometry as input and compare designs on a common basis. They require calibration to test data before they predict cycles to failure, and the NREL slides reviewed give strain energy density and no cycle count.80 Wang and Blaabjerg’s review places physics-of-degradation and mission-profile approaches among the current directions of power electronics reliability research.81

5. Evidence That Low-CTE Baseplates and Cold Plates Extend Module Life

5.1 Modeling favors AlSiC by a factor of 11 to 27 in strain energy density

NREL has modeled the strain energy density per thermal cycle in a power module stack for baseplates of copper, AlSiC and aluminum. In a 2020 presentation the values for a 5 mm baseplate are 3.02 MPa for copper, 0.22 MPa for AlSiC and 6.00 MPa for aluminum.82 In later NREL slides the values for the same thickness are 1.94, 0.18 and 3.93 MPa.83 The ratio of copper to AlSiC is 13.7 in the first set and 10.8 in the second, and the ratio of aluminum to AlSiC is 27.3 and 21.8.84 The two sets differ because the model conditions differ, and the text extracted from the slides does not state the ceramic or the thermal loading.

Figure 4. Strain energy density per cycle by baseplate material and thickness

Strain energy density per cycle by baseplate material and thickness

Values as reported in NREL slides on substrate-attach reliability; the ceramic and loading are not stated in the text retrieved. Bar labels show MPa per cycle.

The strain energy density of the AlSiC baseplate stays at 0.18 MPa from 3 to 6 mm, while copper rises from 1.24 to 2.19 MPa and aluminum from 2.28 to 4.58 MPa (Figure 4).85 Thinner copper and aluminum baseplates reduce the strain energy and leave it above the AlSiC value at every thickness listed. A second NREL slide set states that an AlSiC baseplate offers superior reliability to copper and aluminum baseplates, mainly because of the low CTE mismatch with the ceramic.86 Strain energy density is a damage indicator, and a fatigue law converts it to cycles. The ratios of 11 to 27 therefore indicate direction and relative severity, and they require a calibrated fatigue law before they become life ratios.

5.2 A tested liquid-cooled AlSiC heat sink reports an improvement of at least 18 times

Pahinkar et al. replace the conventional stack of direct bonded copper substrate, solder, copper baseplate, thermal grease and aluminum heat sink with a copper circuit layer on an aluminum nitride dielectric, a transient liquid phase bond and a 3 mm AlSiC heat sink with integrated cooling features.87 Sixteen bonded samples completed 1,800 thermal cycles from −40 to 150 °C and 1,400 hours of aging at 150 °C with no change in void fraction and no failure, cracking or delamination. The authors report a thermal cycling improvement of more than a factor of 18 and, in their conclusion, a lifetime improvement of at least 18 times under the test conditions.88

The comparison baseline and its cycles to failure are not in the text retrieved. If the factor of 18 compares cycles to failure and the test stopped at 1,800 cycles without failure, the conventional stack failed at about 100 cycles or fewer.89 The paper is an undated accepted manuscript. The result applies to a bonded stack that omits the solder layer between substrate and baseplate, so the improvement combines the effect of CTE matching and the effect of removing the baseplate solder joint.

The thermal result matters for a jet-impingement design. At 400 W with 50/50 water-glycol at 80 °C, the maximum device temperature rise above the coolant was 36 °C for 2 mm channels, 38 °C for pin fins and 40 °C for jet impingement, against 36 to 39 °C for a conventional copper and aluminum design from earlier work.90 The jet design operated at a heat transfer coefficient of 57 kW/m²·K, a pressure drop of 40 kPa and a mass flow of 0.094 kg/s.91 The authors conclude that the AlSiC designs are competitive with the conventional design.

5.3 Low-CTE materials conduct less heat than copper

AlSiC conducts 180 W/m·K against 401 W/m·K for copper, and Pahinkar et al. note that AlSiC alone has higher thermal resistance than thick copper, which the integrated cooling offsets.9293 A patent for a carbon fiber and copper heat sink material reports a CTE of 4 to 6 ppm/K against 16.5 ppm/K for pure copper and a thermal conductivity that is not significantly higher than that of silicon.94 Oddone and Reich report a pitch-based carbon fiber composite in aluminum and magnesium matrices with fibers distributed in the plane of the plate. The in-plane CTE can be tuned down to 3 ppm/K and the in-plane thermal conductivity approaches 200 W/m·K, and the through-plane conductivity decreases as the fiber content increases.95 The fibers in that work have a stated conductivity of 900 W/m·K.96 These sources show that a low-CTE plate trades some conductivity for expansion matching, and that fiber orientation determines which direction conducts heat.

5.4 Patents record the design windows used in industry

Three patents state the CTE targets that module designers apply. One power module patent states that the CTE difference between the substrate and the baseplate may be 5, 3 or 2 ppm/K or lower, notes that typical baseplates expand at about 18 ppm/K and that metal matrix composite baseplates expand at about 8 to 9 ppm/K, and prefers a baseplate CTE above that of the substrate.97 A second patent for a SiC module specifies a base plate CTE of 4 to 5.1 ppm/K, with the lower bound set by the CTE of SiC, and an AlSiC heat sink plate of about 7.5 ppm/K.98 A third limits the baseplate and conductive circuit layer to a CTE below 8×10⁻⁶ per °C and a density below 4 g/cm³.99 Patents record claimed designs, and none of these three reports life data.

Table 6. Evidence on the effect of low-CTE materials on power module life

Evidence Type Result Conditions and limits
NREL parametric design study (2020)100 Finite-element modeling Strain energy density per cycle at 5 mm: copper 3.02, AlSiC 0.22, aluminum 6.00 MPa Ceramic and loading not stated in the text retrieved; no cycles to failure
NREL substrate-attach slides101 Finite-element modeling At 5 mm: copper 1.94, AlSiC 0.18, aluminum 3.93 MPa; AlSiC constant from 3 to 6 mm Same limits; conditions differ from the 2020 values
NREL packaging materials slides102 Presentation statement AlSiC baseplate offers superior reliability, mainly through low mismatch with the ceramic Test conditions and cycle counts not retrieved
Pahinkar et al.103 Test, 16 bonded samples No failure at 1,800 cycles, −40 to 150 °C; improvement of at least 18 times Baseline not retrieved; bonded stack omits the baseplate solder joint; undated manuscript
Choe et al.104 Test, 2 samples per combination Silicon nitride substrate survived 1,000 cycles; alumina and aluminum nitride fractured by 10 cycles −50 to 250 °C with 30 min dwell; substrate ceramic only, not baseplate
Hu et al.105 Model validated on silicon modules Stiffness dominates over CTE in SiC die-attach stress Shows that CTE alone does not set solder stress in SiC
Vincotech106 Vendor technical paper Highest stress in the copper baseplate to substrate joint; baseplate bowing and grease pump-out Vendor reasoning; no life figures in the text retrieved
Three U.S. patents107 Design practice Substrate to baseplate CTE difference of 5, 3 or 2 ppm/K or lower; baseplate CTE of 4 to 5.1 ppm/K Claimed designs; no life data

Strain energy density values are reported by NREL. The ratios discussed in the text are derived in this paper.

5.5 The public record has four gaps

  • No source reviewed reports a module-level life test that varies cold plate or baseplate CTE in a SiC module and holds the other variables constant.

  • The modeling results give strain energy density without a calibrated cycles-to-failure relation for the baseplate joint, and the conditions of the two NREL data sets differ.

  • The tested AlSiC heat sink removes the baseplate solder joint, so its result cannot be assigned to CTE alone.

  • No source reviewed reports the in-plane CTE of a carbon fiber composite with fibers oriented through the thickness of the plate.

6. Qualification Standards and What They Test

6.1 AQG 324 defines the module-level lifetime tests

The ECPE guideline AQG 324 is the qualification reference that the Wolfspeed white paper applies. It is based on the German standard LV324 and targets power converter units in vehicles of up to 3.5 tons.108 Its lifetime tests include short-pulse power cycling (QL-01, PCsec), which targets bond-wire breakage and die-attach degradation, and long-pulse power cycling (QL-02, PCmin), which targets solder fatigue between the substrate and the baseplate. Its environmental tests include a thermal shock test (QE-01, TST).109 A Wolfspeed white paper defines PCsec as pulses under 5 s and PCmin as pulses over 15 s, cites typical temperature swings of 75 to 125 °C with maximum junction temperatures of 125 to 175 °C, and reports the failure criteria of a 5 percent rise in drain-source voltage and a 20 percent rise in thermal resistance.110 The same paper states that power cycling has no fixed pass or fail cycle count.111

The pages retrieved do not give the thermal shock temperature range or cycle count of AQG 324, its revision status or its SiC-specific content. The full guideline is available from ECPE and was not obtained for this paper. Any CF-JET test plan that cites AQG 324 requires the current revision and its thermal shock conditions.

6.2 IEC and JEDEC documents define the test methods

IEC 60749-34-1:2025, published in June 2025, describes a test method for determining the capability of power semiconductor modules to withstand the thermal and mechanical stress produced by cycling the power dissipation of the internal semiconductors and the internal connectors. The catalog entry states that details of the method can follow an application guideline such as AQG 324 and that the test causes wear-out and is destructive.112 JEDEC JESD22-A104F.01, dated April 2023, covers temperature cycling in air or another gas in single-, dual- and triple-chamber equipment for component and solder interconnection testing, and its scope excludes thermal shock conditions with the fast ramp rates of liquid-coupled chambers.113 A test laboratory describes JESD22-A106 as the thermal shock method with rapid liquid or air transfer.114 The JEDEC documents address component and solder interconnection reliability, and the pages retrieved give no SiC-specific criteria.

6.3 MIL-STD-810H Method 503.7 applies to the vehicle, and it sets no module conditions

MIL-STD-810H Method 503.7 determines whether materiel can withstand sudden changes in air temperature, and it defines a shock as an air temperature change greater than 10 °C within one minute.115 Transfer between chambers should take no more than one minute, and chamber ramps to the extreme should not exceed 3 °C per minute.116 The method offers four procedures, from a single one-way shock (I-A) to multi-cycle shocks (I-C, with a minimum of three shocks at each condition) and shocks to or from ambient (I-D), and it sets no default temperature extremes. The levels come from field data, requirements documents or the life cycle environmental profile.117 The method lists differential contraction or expansion rates of dissimilar materials among the causes of failure, and it does not use the term CTE.118

Table 7. Standards that apply to thermal cycling qualification of SiC power modules

Standard Test Conditions stated in the sources reviewed Failure criterion Failure mode addressed
AQG 324, QL-01119 Short-pulse power cycling (PCsec) Pulse under 5 s; typical swing 75 to 125 °C; maximum junction temperature 125 to 175 °C120 +5% VDS; +20% Rth Bond wire, die attach
AQG 324, QL-02 Long-pulse power cycling (PCmin) Pulse over 15 s Same Substrate-to-baseplate solder
AQG 324, QE-01 Thermal shock test (TST) Temperature range and cycle count not on the pages retrieved Not retrieved Substrate and joints
IEC 60749-34-1:2025121 Power cycling test method for modules Details may follow an application guideline such as AQG 324 Not retrieved Wear-out of semiconductors and internal connectors
JESD22-A104F.01122 Temperature cycling in air Single, dual or triple chamber; conditions not retrieved Not retrieved Component and solder interconnection
JESD22-A106123 Thermal shock Rapid liquid or air transfer; conditions not retrieved Not retrieved Fast-ramp thermal shock
MIL-STD-810H, Method 503.7124 Air temperature shock Change over 10 °C within 1 min; transfer within 1 min; levels from field data or the life cycle profile Materiel-level; not module-specific Differential expansion of dissimilar materials

Failure criteria of AQG 324 are reported by the Wolfspeed white paper (vendor). Standards catalog entries and vendor pages are the sources for items marked not retrieved.

The standards divide the work. AQG 324 and IEC 60749-34-1 qualify the module, JESD22-A104 qualifies the component and solder interconnection, and MIL-STD-810H qualifies the vehicle or equipment in its mission environment. None of the documents in Table 7 states a cycle count for an Army ground vehicle mission, and the sources reviewed contain no public Army mission profile that defines the number or amplitude of junction temperature cycles.

7. Implications for the CF-JET Effort

The reliability case for a CF-JET module rests on one proposition that the published record supports in direction and leaves unquantified in magnitude: a cooled base with a CTE close to that of the substrate ceramic lowers the strain on the substrate-to-baseplate joint. The CF-JET proposal places a carbon fiber target plate under each die and an electroplated coolant face over it.125 The independent evidence in Table 6 covers AlSiC and ceramic substrates. It covers no carbon fiber target plate.

7.1 Six risks follow from the evidence

  • Fiber orientation. The composites in the literature that combine low CTE with high in-plane conductivity place pitch-based fibers in the plane of the plate.126 The CF-JET proposal orients fibers perpendicular to the plate under each die.127 The sources reviewed report no measured in-plane CTE for a composite with through-thickness fibers, so the CTE that sets the mismatch with the substrate is unquantified.

  • Plated coolant face. A thin electroplated metal layer adds a high-CTE layer (copper at 16.5 ppm/K, Table 2) to a low-CTE plate. In the closest analog found, nickel-phosphorus layers about 7 µm thick on silicon nitride cracked within 1,000 cycles from −50 to 250 °C and nickel layers did not.128 The chemistry and thickness of the CF-JET face require test.

  • Joint between the plate and the metal body. The proposal does not state the body alloy in the sources reviewed. For bodies of copper or aluminum at 16.5 to 25 ppm/K and plates at 3 to 8 ppm/K, the free mismatch at that joint is 8.5 to 22 ppm/K, as large as the die-attach and ceramic joints in Table 3.129

  • Conductivity penalty. AlSiC conducts less than half the heat of copper, and a carbon fiber and copper material has been reported at a conductivity not significantly above silicon.130131 The AlSiC jet design in Pahinkar et al. stayed within about 1 K of the conventional design’s upper value at 400 W, which shows that integrated cooling can offset the penalty. CF-JET must show the same with its own plate.132

  • Coolant temperature range. The future engine coolant requirement of 105 °C raises the mean temperature of the baseplate-side joint, and the cycle at that joint includes the coolant temperature change between cold start and operating temperature.133 The validity limit of 127 °C on mean junction temperature in the Semikron Danfoss model leaves 22 K above a 105 °C coolant, so published models cover the CF-JET operating range only partly.134

  • Qualification basis. AQG 324 is an automotive guideline, and the sources reviewed contain no Army equivalent or mission profile. A CF-JET reliability claim therefore needs a stated cycle definition and failure criterion, because lifetimes stated with different criteria (+5% VDS or +20% Rth) cannot be compared.

7.2 Seven design implications for the program

  • Measure CTE on the finished plate. Report the in-plane and through-thickness CTE and thermal conductivity of the carbon fiber target plate with its plated face, from 25 to 175 °C, with the fiber volume fraction and matrix stated.

  • Select the ceramic and the plate as a pair. Use the method in Table 3 to compute the free mismatch for each candidate, because silicon nitride matches the SiC die best and has a larger mismatch with an AlSiC-like base (5.2 ppm/K) than alumina does (0.2 ppm/K). Patent windows of 2 to 5 ppm/K between substrate and baseplate give a screening range.135

  • Compute strain energy density with a common model. Model the CF-JET stack, an AlSiC stack and a copper stack with the same ceramic and loading, and use the NREL values of 0.18 MPa (AlSiC) and 1.94 MPa (copper) at 5 mm as a check on the model and not as a target, because the NREL conditions are not fully stated.136

  • Test controlled pairs. Build modules that differ only in the cooled base (copper, AlSiC, CF-JET) so that the result separates the effect of CTE from the effect of removing the baseplate solder joint, which the tested AlSiC heat sink did not separate.137

  • Define the cycles and the criteria. Apply power cycling with swings of 75 to 125 °C and maximum junction temperatures to 175 °C, both pulse regimes (under 5 s and over 15 s), and the AQG 324 thermal shock test at its current conditions. Report both failure criteria (+5% VDS and +20% Rth).138

  • Monitor thermal resistance every cycle. Wolfspeed computes thermal resistance each cycle from the body diode forward voltage during the off time, which tracks joint degradation throughout the test.139 The same monitoring applies to a CF-JET module.

  • State the model conditions with every lifetime. Report the failure criterion, the failure probability level (the Semikron Danfoss figures represent 15 percent) and whether the test conditions lie inside the validity ranges of the model used.140

7.3 Six research questions remain open

  • What in-plane CTE does a pitch-based carbon fiber plate with through-thickness fibers have as a function of fiber volume fraction and matrix, and how does it change from 25 to 175 °C?

  • Does an electroplated face of a given metal, chemistry and thickness survive more than 1,000 thermal shock cycles on that plate without cracking or delamination?

  • How does the strain energy density of a SiC module on a CF-JET plate compare with AlSiC (0.18 MPa) and copper (1.94 MPa) for the same ceramic and loading?

  • How many junction and baseplate-joint temperature cycles, at what amplitude, does an Army ground vehicle mission impose with 105 °C coolant and engine-off operation?

  • What calibrated fatigue law converts the strain energy density ratios of 11 to 27 into life ratios for the baseplate joint?

  • Does a CTE-matched cooled base move the dominant failure to the next-weakest interface, such as the bond wire or die attach, so that further life gains from the cold plate saturate?

8. Conclusion

CTE mismatch between SiC dies, ceramics, joining layers and metal baseplates is a leading wear-out driver in SiC power modules that cycle in temperature. Copper and aluminum expand four to eight times as much as SiC and silicon nitride, and the joining layers experience the largest free mismatch. SiC adds stiffness that raises the stress in die-attach solder, and the published comparison attributes that effect mainly to elastic modulus.

The lifetime models in common use express life through junction temperature swing and contain no CTE term. Only finite-element and physics-of-failure models take CTE as input. The evidence that a low-CTE base extends life consists of NREL modeling that favors AlSiC by a factor of 11 to 27 in strain energy density, one tested AlSiC liquid-cooled heat sink with a reported improvement of at least 18 times, and substrate-level tests. No published test varies cold plate CTE alone in a SiC module.

The CF-JET effort can contribute that evidence. It requires measured in-plane CTE of the finished target plate, a ceramic and plate pairing selected by computed mismatch, controlled comparison modules, and power cycling and thermal shock tests with the AQG 324 failure criteria and a stated cycle definition.

Bibliography

Accendo Reliability. “Norris-Landzberg.” Trade web page. Accessed 23 November 2026. https://accendoreliability.com/tag/norris-landzberg/.

Bayerer, Reinhold, Thomas Licht, Tobias Herrmann, Josef Lutz, and Marco Feller. “Model for Power Cycling Lifetime of IGBT Modules – Various Factors Influencing Lifetime.” Paper presented at CIPS 2008, 5th International Conference on Integrated Power Electronics Systems, Nuremberg, 11–13 March 2008. https://vde-verlag.de/proceedings-en/453089004.html.

Choe, Chanyang, Chuantong Chen, Seungjun Noh, and Katsuaki Suganuma. “Thermal Shock Performance of DBA/AMB Substrates Plated by Ni and Ni–P Layers for High-Temperature Applications of Power Device Modules.” Materials 11, no. 12 (28 November 2018): 2394. https://doi.org/10.3390/ma11122394.

Escobar, Luis A., and William Q. Meeker. “A Review of Accelerated Test Models.” arXiv:0708.0369, 2007. https://doi.org/10.1214/088342306000000321.

Held, M., et al. “Fast Power Cycling Test of IGBT Modules in Traction Application.” Paper presented at the International Conference on Power Electronics and Drive Systems (PEDS), 1997. Indexed at Fraunhofer Publica. https://publica.fraunhofer.de.

Hu, Borong, Jose Ortiz Gonzalez, Li Ran, Hai Ren, Zheng Zeng, Wei Lai, Bing Gao, Olayiwola Alatise, Hua Lu, Christopher Bailey, and Phil Mawby. “Failure and Reliability Analysis of a SiC Power Module Based on Stress Comparison to a Si Device.” IEEE Transactions on Device and Materials Reliability 17, no. 4 (December 2017): 727–37. https://doi.org/10.1109/TDMR.2017.2766692.

Infinita Lab. “JESD22-A104 Temperature Cycling Testing for Semiconductors.” Test laboratory web page. Accessed 23 November 2026. https://infinitalab.com/services/jesd22-a104-temperature-cycling-testing/.

International Electrotechnical Commission. IEC 60749-34-1:2025, Semiconductor Devices – Mechanical and Climatic Test Methods – Part 34-1: Power Cycling Test for Power Semiconductor Module. Edition 1.0, June 2025. Catalog entry at https://www.vde-verlag.de/iec-normen/255200/iec-60749-34-1-2025.html.

Izquierdo Gomez, Pere, Miguel E. Lopez Gajardo, Nenad Mijatovic, and Tomislav Dragicevic. “A Self-Commissioning Edge Computing Method for Data-Driven Anomaly Detection in Power Electronic Systems.” arXiv preprint, 5 December 2023. https://arxiv.org/abs/2312.02661.

JEDEC Solid State Technology Association. JESD22-A104F.01, Temperature Cycling. April 2023. Catalog entry at https://standards.globalspec.com/std/14597601/jesd22-a104f-01.

Kozak, Joseph P., Douglas J. DeVoto, Joshua J. Major, and Khai D. T. Ngo. “Trends in SiC MOSFET Threshold Voltage and ON-Resistance Measurements from Thermal Cycling and Electrical Switching Stresses.” NREL/CP-5400-70550. Paper presented at the 10th International Conference on Integrated Power Electronics Systems, Stuttgart, 20–22 March 2018. https://www.nrel.gov/docs/fy18osti/70550.pdf.

Künzi, R. “Thermal Design of Power Electronic Circuits.” Lecture notes, Paul Scherrer Institute. arXiv:1607.01578. https://arxiv.org/pdf/1607.01578.

Matsusada Precision. “AQG 324 Test Standard.” Vendor web page. Accessed 23 November 2026. https://www.matsusada.com/application/ps/aqg324/.

National Renewable Energy Laboratory. Presentation slides on substrate-attach reliability and baseplate and ceramic material selection. NREL document fy22osti/79098, n.d. https://www.nrel.gov:443/docs/fy22osti/79098.pdf.

National Renewable Energy Laboratory. Presentation slides on high-temperature packaging materials, including the effect of baseplate and ceramic material. NREL document fy22osti/81341, n.d. https://www.nrel.gov:443/docs/fy22osti/81341.pdf.

Oddone, Valerio, and Stephanie Reich. “Thermal Properties of Metal Matrix Composites with Planar Distribution of Carbon Fibres.” Free University of Berlin, undated manuscript. https://core.ac.uk/download/199419104.pdf.

Pahinkar, Darshan G., Lauren Boteler, Dimeji Ibitayo, Sreekant Narumanchi, Paul Paret, Douglas DeVoto, Joshua Major, and Samuel Graham. “Liquid Cooled Aluminum Silicon Carbide Heat Sinks for Reliable Power Electronics Packages.” Accepted manuscript, U.S. Department of Energy Public Access, undated. https://www.osti.gov/servlets/purl/1507288.

Paret, Paul. “Parametric Design Study of a Power Electronics Package.” Presentation, IEEE ITherm Conference, 21–23 July 2020. National Renewable Energy Laboratory. https://www.nrel.gov:443/docs/fy20osti/77235.pdf.

Rogers Corporation. curamik Ceramic Substrates. Vendor technical data sheet, n.d. https://www.RogersCorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/data-sheets/technical-data-sheet-curamik-ceramic-substrates.pdf.

SOL Engineering Services, LLC. CF-JET: AI/ML-Enabled Design and Development of an Additively Manufactured, Liquid-Cooled Jet-Impingement Cold Plate with Optimized Carbon Fiber Target Plate. Proposal, Rev Final 2, n.d.

Texas Instruments. “Solder Joint Reliability Acceleration Model.” E2E support forum thread. Accessed 23 November 2026. https://e2e.ti.com/support/data-converters-group/data-converters/f/data-converters-forum/730473/solder-joint-reliability-acceleration-model.

U.S. Army Combat Capabilities Development Command, Ground Vehicle Systems Center. “GVSC Planned Combat Vehicle Electrification and Mobility Programs (CVEMP).” Briefing, 30 May 2019. https://apps.dtic.mil/sti/pdfs/AD1080428.pdf.

U.S. Department of Defense. MIL-STD-810H, Method 503.7, Temperature Shock. 31 January 2019. Copy of the method at https://www.trentonsystems.com/hubfs/mil-std-810h-temp-shock.pdf.

“Method of Converting Power Using a Power Semiconductor Module.” U.S. Patent 8,889,458. U.S. Patent and Trademark Office. https://patents.justia.com/patent/8889458.

“Method for Fabricating a Heat Sink, and Heat Sink.” U.S. Patent 10,017,870. U.S. Patent and Trademark Office. https://image-ppubs.uspto.gov/dirsearch-public/print/downloadPdf/10017870.

“Power Semiconductor Module Arrangement.” U.S. Patent 10,879,148. U.S. Patent and Trademark Office. https://image-ppubs.uspto.gov/dirsearch-public/print/downloadPdf/10879148.

“Semiconductor Device.” U.S. Patent 11,043,465. U.S. Patent and Trademark Office. https://image-ppubs.uspto.gov/dirsearch-public/print/downloadPdf/11043465.

Vasudevan, Vasu, and Xuejun Fan. “An Acceleration Model for Lead-Free (SAC) Solder Joint Reliability under Thermal Cycling.” Paper presented at the 2008 Electronic Components and Technology Conference. https://www.lamar.edu/engineering/_files/documents/mechanical/dr.-fan-publications/2008/Fan%202008_13%20ECTC_3.pdf.

Vincotech. “Modules without Base Plate.” Vendor technical paper TP 2012-03-001, v01, n.d. https://www.vincotech.com/fileadmin/user_upload/content_media/documents/pdf/support-documents/technical-papers/TP_2012-03-001-v01_Modules_without_base_plate.pdf.

Wang, Huai, and Frede Blaabjerg. “Power Electronics Reliability: State of the Art and Outlook.” IEEE Journal of Emerging and Selected Topics in Power Electronics 9, no. 6 (December 2021): 6476–93. https://doi.org/10.1109/JESTPE.2020.3037161.

Wintrich, Arendt. Power Cycle Model for IGBT Product Lines. Application note AN 21-001, rev. 02. Semikron Danfoss, 23 July 2024. https://assets.danfoss.com/documents/latest/444233/AB501650017495en-000201.pdf.

Wolfspeed. “SiC Power Module Reliability: Wolfspeed Power Cycling and Lifetime Modeling Approach.” Vendor white paper, 14 November 2025. https://assets.wolfspeed.com/uploads/2025/11/Wolfspeed_Power_Cycling_and_Lifetime_Modeling_Approach.pdf.

Yang, Shaoyong, Angus Bryant, Philip Mawby, Dawei Xiang, Li Ran, and Peter Tavner. “An Industry-Based Survey of Reliability in Power Electronic Converters.” IEEE Transactions on Industry Applications 47, no. 3 (May 2011): 1441–51. https://doi.org/10.1109/TIA.2011.2124436.

Notes

ESC
CITE ·